Skip to main content

Table 1 Composition of plating solution and experimental parameters

From: Efficient Preparation of Nanoparticle-Reinforced Nickel-based Composite Coating with Highly Preferred (220) Orientation

Composition and parameters

Quantity

NiSO4·6H2O (g/L)

300

NiCl2·6H2O (g/L)

40

H3BO4 (g/L)

40

Saccharin (g/L)

0.5

Emulsifier OP-10 (g/L)

1.0

SiC nano-particles (g/L)

3.0

pH value

4.0

Nozzle diameter (mm)

5.0

Scanning speed of nozzle (mm/min)

100

Distance between nozzle and cathode (mm)

3.0

Injection velocity (m/s)

1.40‒2.65

Current density (A/dm2)

180‒220

Temperature (°C)

60