Table 6 Experimental parameters comparison of T25 and T26

From: Face Grinding Surface Quality of High Volume Fraction SiCp/Al Composite Materials

Parameter

T25

T26

Feeding amount (mm/min)

100

100

Grinding depth (μm)

5

20

Spindle speed (r/min)

6000

6000

F

1.55

2.75

COF

0.17

0.22

Sdr

1.13

1.09

Ra

2.39

2.44

Rab

0.31

0.32

Rp

13.80

22.77

Rv

14.3

17.01

Ssk

−0.16

−0.4

Sku

2.70

3.39