From: Study of Cracking Mechanism and Wear Resistance in Laser Cladding Coating of Ni-based Alloy
Location | B | C | Cr | Fe | Ni | W | Si |
---|---|---|---|---|---|---|---|
A | 10.45 | 6.08 | 31.26 | 39.06 | 9.79 | 1.14 | Â |
B | Â | 9.7 | 15.93 | 33.62 | 34.36 | Â | 2.24 |
C | Â | 7.83 | 4.23 | 34.64 | 47.19 | Â | 3.42 |
D | 7.16 | 9.13 | 9.67 | 66.11 | 7.37 | 0.29 | 0.27 |
E | Â | 10.35 | 5.01 | 68.58 | 14.79 | Â | 1.27 |
F | Â | 8.64 | 5.06 | 71.42 | 13.79 | Â | 1.09 |