From: Effect of Surface Texture on Tensile Shear Strength of 1060Al-PET Welding Joints
Factor | Marking defocusing A (mm) | Marking times B | Results (MPa) |
---|---|---|---|
Test 1 | 0 | 2 | 35.79 |
Test 2 | 0 | 5 | 39.44 |
Test 3 | 0 | 8 | 41.69 |
Test 4 | 0 | 12 | 47.08 |
Test 5 | 0 | 15 | 46.98 |
Test 6 | 1 | 2 | 37.70 |
Test 7 | 1 | 5 | 34.58 |
Test 8 | 1 | 8 | 42.98 |
Test 9 | 1 | 12 | 46.36 |
Test 10 | 1 | 15 | 41.10 |
Test 11 | 3 | 2 | 39.18 |
Test 12 | 3 | 5 | 41.66 |
Test 13 | 3 | 8 | 46.90 |
Test 14 | 3 | 12 | 44.09 |
Test 15 | 3 | 15 | 43.11 |
Test 16 | 5 | 2 | 38.01 |
Test 17 | 5 | 5 | 39.73 |
Test 18 | 5 | 8 | 44.02 |
Test 19 | 5 | 12 | 43.33 |
Test 20 | 5 | 15 | 40.26 |
Average value 1 | 42.1 | 38.1 | |
Average value 2 | 40.8 | 38.2 | |
Average value 3 | 41.8 | 42.9 | |
Average value 4 | 41.1 | 43.3 | |
Average value 5 | 41.6 | ||
Range | 1.3 | 5.2 | |
Optimal combination | A1B4 |